Loading simulation data

Battery thermal management · Phase change material

How thick should the PCM wrap around a battery cell be?

An 18650 cell, a ring of RT-42 paraffin 6, 8 or 10 mm thick, and an acrylic shell. 56 transient simulations, checked against a published study, to see which layer keeps the cell coolest and what each extra millimetre buys.

Bare cell25.0 °C
3C discharge0 s
8 mm PCM25.0 °C
25 °C90 °C
0°C peak on a bare cell after 1200 s at 3C
0°C with an 8 mm PCM wrap, same load
0K separates 6 mm from 10 mm at 3C
0K worst gap to the published results

01 · The problem

One cell, three wraps

The cell is the same 18 × 65 mm cylinder used in the reference study. It generates heat as I²R. Around it sits an annulus of paraffin, then a 2 mm acrylic shell. Air cools the top and the outer wall. The base is insulated.

Li-ion cell

ρ
2720 kg/m³
cp
300 J/kg·K
k
3.0 W/m·K
q at 2C / 3C
0.69 / 1.56 W

RT-42 paraffin

ρ
820 kg/m³
cp
2000 J/kg·K
k
0.2 W/m·K
Latent heat
165 kJ/kg
Melts
38 to 43 °C

Acrylic shell

ρ
1215 kg/m³
cp
1300 J/kg·K
k
0.17 W/m·K
Thickness
2 mm

Boundaries

Top + side
h = 5.7 W/m²K
Air
25 °C
Bottom
insulated
Start
25 °C

Inputs from Alma'asfa et al. 2025 J. Therm. Anal. Calorim. 150:12643. The paper fixes the PCM at 8 mm. This study varies it.

02 · Can we trust it?

Matches the published study within 1.1 K

Before comparing thicknesses, the model had to reproduce the paper's own numbers. The bare cell and the 8 mm case appear in both, so they are the test. Melting also starts at 564 s here against roughly 580 s in the paper.

Peak surface temperature at 1200 s

Side by side

The paper reports the 8 mm, 3C result only as a 51.24% reduction. That works out to 41.35 °C.

03 · Field explorer

Watch the heat move

Every frame below is the simulated temperature field, every 20 s of the discharge. Drag the 3D model to look around the cut. Switch to the melt view to see where the paraffin turns liquid.

3D cut-away · drag to rotate
r-z section
Time0 s
Max cell surface25.0 °C
Hottest point in cell25.0 °C
PCM melted0.0 %
Heat stored as latent0 J
25 °C45 °C

04 · Results at h = 5.7 W/m²K, 25 °C

All three wraps work. The gaps between them are small.

Any PCM layer cuts the 3C peak roughly in half. Going from 6 to 10 mm buys another 0.8 K at 3C and 1.7 K at 2C, while the paraffin mass almost doubles from 24 g to 47 g.

Max cell surface temperature

Shaded band is the RT-42 melting range. Hover for values.

Peak at 1200 s

How much PCM melts

Where the heat went by the end of discharge

Share of all heat the cell generated. Hover a segment for joules.

Lowest temperature

10 mm

Coolest in every case simulated, by under a kelvin at 3C.

Best per gram

6 mm

98% of the 10 mm cooling at 3C with half the paraffin, and it melts the most of its own mass.

Paper's pick

8 mm

Sits in between on both counts.

The bigger finding. At 2C and 25 °C none of the wraps reaches 38 °C, so no paraffin melts at all. The latent heat that is the whole point of a PCM goes unused, and the layer acts only as extra thermal mass.

05 · Sensitivity

Airflow and room temperature matter more than thickness

The same designs with stronger convection, and in a warmer room where the cell starts at the ambient temperature.

Peak at 1200 s against h

Peak at 1200 s against ambient

06 · Try it

Run your own design

This is the same solver used for the report, compiled for your browser. It reproduces the report's numbers to within 0.005 K. Change anything and it re-runs in about a second, alongside a bare cell under the same conditions.

PCM properties
Peak surface-
Rise cut vs bare-of the temperature rise
Melt starts-
Paraffin mass-

Field at the end of the run

07 · Insulator or heat spreader?

At this size the wrap helps the cell shed heat

For a cylinder, an added layer raises heat loss until its outer radius reaches the critical radius rc = k/h. For RT-42 in still air that is 35 mm. Every design here ends between 17 and 21 mm, so in continuous use a thicker wrap lets the cell run cooler.

Steady heat loss per metre of cell against outer radius

Cell surface held at 45 °C, air at 25 °C. Move the sliders.

Where the cell would settle in continuous operation

Steady state, PCM fully molten, conduction only (an upper bound).

08 · How it was solved

The model and the factors that matter

Governing equation

∂H/∂t = (1/r) ∂/∂r ( k r ∂T/∂r ) + ∂/∂z ( k ∂T/∂z ) + q
H = ρcpT + ρLβ(T), β = (T − 38)/(43 − 38) clipped to [0, 1]

A 2D axisymmetric finite-volume model in r and z. The paraffin uses the enthalpy method, the same formulation as Fluent's Solidification & Melting model. Faces line up with every material boundary, and heat flux is continuous across them. Time stepping is explicit at 0.059 s.

Liquid paraffin is treated as conducting only. The Rayleigh number across the full gap is 356 to 1649, and the real molten film is 2 to 2.5 mm thick, which puts it below 50. Natural convection there is negligible.

Grid independence (8 mm, 3C)

From 448 to 30,160 cells the peak moves by 0.08 K. The working grid of 1,885 cells is within 0.021 K of the finest. The energy balance closes to better than 1e-14 of the heat generated.

Assumptions worth knowing

  • Cell heat capacity of 300 J/kg·K is kept from the paper so results stay comparable. Real 18650 cells sit around 900 to 1100, which would slow every rise.
  • Constant I²R heat with 30 mΩ. Real heat generation climbs near the end of discharge.
  • Isotropic cell conductivity. A real jelly roll conducts far better along its axis.
  • No radiation or contact resistance, as in the paper.
  • Single cell in open air. In a pack, neighbours share PCM and see much less airflow.

Rebuilding it in ANSYS Fluent

Settings
Geometry
2D axisymmetric, or 3D as in the paper
Models
Energy, Solidification & Melting (mushy constant 1e5), laminar
PCM
Boussinesq ρ 820, β 1e-4, cp 2000, k 0.2, μ 0.02, L 165000, solidus 311.15 K, liquidus 316.15 K
Cell source
41,788.37 W/m³ (2C) or 94,023.84 W/m³ (3C)
Walls
Top and outer: convection h 5.7, 298.15 K. Bottom: q = 0
Solver
SIMPLEC, PRESTO!, second-order upwind, Δt 0.5 s
PDF
Full report14 pages, every table and figure
PY
Solver and scriptssim.py, run_all.py, plots, results
REF
Reference studyAlma'asfa et al. 2025, J. Therm. Anal. Calorim. 150:12643